Properties of Novilon materials- Novilon Grafoil

Properties Method of
testing
Unit Novilon Grafoil
PA 6 G+oil+grafit
MECHANICAL
* tensile strength ISO 527 MPa 69-71
* flexural strength ISO 178 MPa 120-122
* compressive strength ISO 604 MPa 106-109
* tensile modulus of elasticity ISO 527 MPa 3360-3600
* flexural modulus of elasticity ISO 178 MPa 2900-3300
* compressive modulus of elasticity ISO 604 MPa 2700-3200
* allowable compression during longer loading time - MPa 18
* impact strenght – notched (CHARPY) ISO 179   5,91
* hardness – Shore D method ISO 868   79-82
* coefficient of friction ASTM D 1894   0,162
THERMAL
melting point ISO 3146 °C 223
* softening temperature (Vicat method) ISO 306 °C 220
working temperature - long period - °C -40 do 110
working temperature - short period - °C 160
* average thermal expansion (23 do 80°C) α ASTM D 696 K-1 10,0·10-5
thermal conductivity ASTM C 177 W/mK -
ELECTRICAL
* dielectricity VDE 0303 Teil4
IEC 250
- 3,5
** dielectric dissipation factor (at 1 MHz) VDE 0303 Teil4
IEC 250
- 0,023
surface resistivity VDE 0303 Teil3
IEC 93
Ω 1,3·1013
** resistivity VDE 0303 Teil3
IEC 93
Ω cm 1,4·1016
electric strenght VDE 0303 Teil2
IEC 243
kV/mm -
Resistance to tracking (CTI) VDE 0303 Teil1
IEC 112
- CTI 450M
OTHER
density ISO 1183 g/cm3 -
* water absorption (changes of weight, 28 days, 65% HR/23°C) INTERNA % 0,053
* water absorption (dimensional changes, 28 days, 65% HR/23°C)   % 0,090
water absorption (long-time exposure on the air 50% HR/33°C) ASTM D 570 % 2-2,5
water absorption (to saturation) ASTM D 570 % 5-6
Specific properties of particular types of Novilon Dobre drsne lastnosti
Povečan dovoljeni pritisk pri dolgotrajni obremenitvi

* TESTED BY FACULTY OF MECHANICAL ENGINEERING AND NAVAL ARHITECTURE - Zagreb
** TESTED BY ISKRA KIBERNETIKA - Kranj